Three plasticizers dominate the C24 region of the catalogue, and buyers confuse them constantly: DEHP (bis(2-ethylhexyl) phthalate, CAS 117-81-7), DOTP (bis(2-ethylhexyl) terephthalate, CAS 6422-86-2) and DEHCH (bis(2-ethylhexyl) cyclohexane-1,2-dicarboxylate, CAS 84-71-9). All three carry two 2-ethylhexyl chains and two ester groups. Two of them are the same molecule written differently; the third is genuinely a different compound. Getting that straight solves most of the sourcing problems in this part of the market.
Start with the atoms, because that settles two of the three questions
| Product | CAS | Formula | MW | Sap. value | Ring |
| DEHP (DOP) | 117-81-7 | C24H38O4 | 390.56 | 287.3 | Benzene, ortho-disubstituted |
| DOTP (DEHT) | 6422-86-2 | C24H38O4 | 390.56 | 287.3 | Benzene, para-disubstituted |
| DEHCH | 84-71-9 | C24H44O4 | 396.61 | 282.9 | Cyclohexane, saturated |
Two observations follow immediately, and both are load-bearing:
- DEHP and DOTP have the same molecular formula, the same molecular weight and therefore the same saponification value. No titration, no mass measurement and no elemental analysis will ever separate them. They differ only in where the second ester group sits on the ring – adjacent (ortho) in DEHP, opposite (para) in DOTP.
- DEHCH is six hydrogens heavier. Hydrogenating the aromatic ring adds three molecules of hydrogen, taking C24H38O4 to C24H44O4 and 390.56 to 396.61 g/mol. That 6.05 g/mol step is the single cleanest way to tell an aromatic C24 ester from a saturated one.
So the first question – “is this product saturated?” – is answered by molecular weight alone. The second question – “which aromatic isomer is it?” – needs a structural method, because no compositional method can help.
What hydrogenation changes
DEHP and DEHCH differ by a ring and nothing else. The alkyl chains are both 2-ethylhexyl, the ester groups are both on adjacent ring carbons, and the molecule’s overall size and shape are almost unchanged. What the saturated ring does change is the electronic structure:
| Property | DEHP / DOTP (aromatic) | DEHCH (saturated) | Consequence |
| Ultraviolet absorbance, 250 to 280 nm | Strong | None | The only cheap test that proves the phthalate ring is gone |
| Refractive index | Higher (pi electrons) | Lower | Rapid screening of a substituted lot |
| Density | Higher (aromatic packing) | Lower | Independent confirmation of the same substitution |
| Solvation of PVC | Stronger | Slightly weaker | A low single-digit higher phr is needed for the same hardness |
| Gelation behaviour | Faster | Marginally slower and hotter | Re-check the fusion window on the line |
| Volatility, migration, extraction | Governed by the 2-ethylhexyl chains and by molecular weight, not by the ring | Do not expect the substitution to fix a permanence problem | |
| Colour stability under light | Can yellow via aromatic absorption | No aromatic chromophore | Matters for clear and white articles |
That last-but-one row is where most of the confusion in the market lives. Hydrogenation is often presented as an upgrade across the board. It is not. It removes an aromatic ring and its consequences – chromophore, slightly denser packing, slightly stronger solvation – and it leaves the durability physics exactly where it was, because those come from chain length.
Ortho versus para: what actually differs
DEHP and DOTP are both aromatic diesters of 2-ethylhexyl alcohol, and on paper they look interchangeable. In a compound they are close but not identical, and the differences trace back to the geometry of the ring:
- Packing and crystallisation. The para arrangement is more symmetric and packs more regularly. That changes the tendency to crystallise or haze at low temperature, and it changes the shape of the viscosity curve.
- Processing position. DOTP is generally used where a non-ortho aromatic ester is required – the “terephthalate” route – and it processes close enough to DEHP that many lines switch without new tooling.
- Regulatory status. The two are separate substances with separate CAS numbers and separate regulatory positions. A restriction written for DEHP does not automatically cover DOTP, and vice versa. That is precisely why the naming matters commercially.
What does not differ is composition. C24H38O4 at 390.56 g/mol is C24H38O4 at 390.56 g/mol, and any specification that stops at those two facts has not distinguished between the two most commonly confused products in this group.
The identification matrix
This table is the practical answer to “how do I know what is in the drum”. Read it as two separate questions, because no single test answers both.
| Method | Separates DEHCH from the aromatic esters | Separates DEHP from DOTP | Notes |
| Molecular weight on the COA | Yes – 396.61 against 390.56 | No | The cheapest check there is; it fails only through dishonesty |
| Saponification value | Yes – 282.9 against 287.3 | No – both 287.3 | A ~4.5 point difference is small but real; identical values prove nothing |
| UV absorbance, 254 to 280 nm | Yes – none against strong | No – both absorb | The most sensitive test for residual aromatic content |
| Refractive index / density | Yes | Weakly | Fast and cheap, but small differences invite arguments |
| Infrared spectroscopy | Yes – no aromatic C-H stretch | Yes – out-of-plane bending near 745 cm-1 (ortho) against 730 cm-1 (para) | The standard fingerprint for substitution pattern |
| Proton NMR | Yes – no aromatic protons | Yes – four adjacent ring protons give a multiplet, para substitution gives two 2H doublets | Definitive, and available at any contract lab |
The commercial lesson: if the only thing on the certificate is assay and colour, you have no evidence about either question. Ask for the molecular weight and the saponification value on the COA – both are inexpensive and both are structural – and reserve IR or NMR for the cases where the substitution pattern actually matters.
Choosing between them
| Requirement | Choice | Reason |
| Lowest cost, general-purpose PVC | DEHP | Unbeatable economics where it is permitted |
| Non-ortho aromatic ester required | DOTP | Same atoms, para geometry, close processing match to DEHP |
| No aromatic ring required | DEHCH | The ring is gone; UV-transparent; no aromatic chromophore |
| Long-service cable or high-temperature ageing | None of the three | Move to a C9 or C10 ester; 390 to 397 g/mol is not enough permanence |
| Low-temperature flexibility | None of the three | An aliphatic adipate such as DOA is the right tool |
| Clear or white article that must not yellow | DEHCH | No aromatic absorption to drive colour development |
The negative rows are as useful as the positive ones. A buyer who arrives with “we need better permanence, and our supplier offered DEHCH” has been offered a regulatory substitution, not a performance one. The C24 esters are a processing class; the C9 and C10 cyclohexane dicarboxylates are the permanence class.
Dose and cost, worked through
Moving from DEHP to DEHCH changes two numbers on the cost sheet, and only one of them is usually quoted:
- Mass per kilogram. DEHCH is 6.05 g/mol heavier, so the same phr buys 1.5% fewer moles of plasticizer. That alone would call for a slightly higher loading.
- Solvating power. The saturated ring solvates PVC less aggressively, which pushes the required loading up by a low single-digit percentage on top of the mass effect.
- Worked example. A compound at 50 phr contains 33.3% plasticizer by mass; if the reformulation lands at 53 phr, the demand per tonne of compound rises from 333 kg to 346 kg. On a 20-tonne order that is 260 kg of extra plasticizer – the number that belongs in the business case.
Against DOTP there is usually no dose penalty at all, because the mass and the solvating behaviour are effectively DEHP’s. That is why DOTP has been the low-friction substitution for formulators who do not need an aromatic-free claim.
Where each one actually goes
| Application | DEHP | DOTP | DEHCH |
| General flexible PVC (where permitted) | Standard | Standard alternative | Standard alternative |
| Cable insulation and sheathing | Legacy use, shrinking | Used, where aromatic is acceptable | Used, especially for colour retention |
| Automotive interior | Restricted or avoided | Used | Used – no chromophore, no aromatic fogging signature |
| Toys and childcare | Excluded in most markets | Used in some markets | Used where an aromatic-free claim is needed |
| Flooring, wall covering | Legacy | Used | Used – colour retention in the wear layer |
| Adhesives, sealants, inks | Legacy | Used | Less common – the dibutyl ester is usually the better fit |
Specifying and verifying
- Put the molecular weight on the purchase order, to two decimal places. It is the difference between 390.56 and 396.61, and no supplier can meet a specification they have not been given.
- Ask for the saponification value. It separates the saturated ester from the aromatic pair, and it catches partial esterification and monoester residue at the same time.
- Ask for UV absorbance on the neat liquid or at a stated dilution, with the path length. A number without the method is not a result.
- Reserve IR or NMR for substitution-pattern disputes. Those are the only routine methods that settle ortho against para, and they settle it conclusively.
- Declare the shipping service for bulk deliveries. A tanker previously carrying a phthalate will leave residue that a UV audit finds – which is exactly what the test is for.
FAQ
Are DEHP and DOTP the same product?
No – and yes, in the sense that matters for a certificate. They are different substances with different CAS numbers and different regulatory positions, but they have the same molecular formula, the same molecular weight (390.56) and the same saponification value (287.3). Only a structural method – infrared or NMR – separates ortho from para.
Is DEHCH simply hydrogenated DEHP?
Chemically, yes: the aromatic ring is saturated and three moles of hydrogen are added per mole of diester, taking the formula from C24H38O4 to C24H44O4. That is why the molecular weight moves by exactly 6.05 g/mol and why the ultraviolet absorbance disappears.
Does DEHCH perform better than DEHP?
Differently, not universally better. It is slightly less efficient and slightly slower to gel, it is UV-transparent, and it has no aromatic chromophore. Volatility, migration and extraction are essentially unchanged because the chains and the molecular weight are unchanged.
How do I prove a delivery is DOTP and not DEHP?
Infrared: look for the aromatic out-of-plane bending band, near 745 cm-1 for the ortho ester and near 730 cm-1 for the para ester. Proton NMR is the definitive alternative – four adjacent aromatic protons give a multiplet, para substitution gives two 2H doublets.
Why does the saponification value matter if the assay is 99%?
Because an assay by gas chromatography normalises the peaks it sees and can pass a lot that contains material it did not resolve. The saponification value is an absolute number fixed by molecular weight and ester count, so it catches wrong-chain and partly esterified material that a normalised purity figure hides.
Contact PolyBlueChem for lot COAs with molecular weight, saponification value and UV absorbance reported, samples of all three C24 grades for side-by-side trials, and a quotation against your volume and destination port.
Related reading
- Cyclohexane dicarboxylate plasticizers: the non-phthalate family selection map
- Verifying a non-phthalate claim: UV absorbance, saponification value and refractive index
- DINCH in toys, medical PVC and food contact: what the specification has to prove
Related products
- Bis(2-ethylhexyl) cyclohexane-1,2-dicarboxylate, DEHCH (CAS 84-71-9)
- Di(2-ethylhexyl) phthalate, DEHP (CAS 117-81-7)
- Di(2-ethylhexyl) terephthalate, DOTP (CAS 6422-86-2)
- Diisononyl cyclohexane-1,2-dicarboxylate, DINCH (CAS 166412-78-8)
- Diisodecyl cyclohexane-1,2-dicarboxylate (CAS 84731-64-6)
- Bis(2-ethylhexyl) adipate, DOA (CAS 103-23-1)