Hydrogenated Bisphenol A (HBPA): Hydroxyl Value, Weathering and the 80-04-6 / 80-05-7 Distinction

Hydrogenated bisphenol A is what bisphenol A becomes when both aromatic rings are carried all the way to cyclohexane: C15H28O2, 240.38 g/mol, a white solid with two secondary hydroxyl groups, a theoretical hydroxyl value of 466.8 mg KOH/g and a hydroxyl equivalent weight of 120.19 g/eq. The molecular weight rises by only 5.3% in the process, and that small change is the whole product.

What the hydrogenation removes is the ultraviolet chromophore. Bisphenol A absorbs strongly in the 270 to 280 nm region because of its two phenolic rings, and a polymer built on it yellows and chalks in exterior service for exactly that reason. The cycloaliphatic rings of HBPA have no absorption in that region, so coatings and castings built on HBPA keep colour and gloss outdoors. Everything HBPA is bought for follows: weatherable saturated polyesters for powder and coil coatings, hydrogenated epoxy resins for exterior and can coatings, low-shrink diacrylate monomers for radiation curing, and non-yellowing polyurethane hard segments.

What Hydrogenation Buys, and What It Costs

Bisphenol A and hydrogenated bisphenol A are the same skeleton with different rings: an isopropylidene bridge joining two six-membered rings, each carrying one hydroxyl. In bisphenol A the rings are benzene and the hydroxyls are phenolic; in HBPA the rings are cyclohexane and the hydroxyls are secondary alcohols.

Property Bisphenol A (80-05-7) Hydrogenated bisphenol A (80-04-6)
Formula C15H16O2 C15H28O2
Molecular weight 228.29 240.38 (+5.3%)
Ring type Aromatic (phenolic OH) Cycloaliphatic (secondary OH)
Hydroxyl equivalent weight 114.14 g/eq 120.19 g/eq (+5.3%)
UV absorption 270-280 nm Strong None
Reaction with epichlorohydrin Direct, via the phenoxide Needs stronger conditions – hence the price of hydrogenated epoxy
Colour on exterior exposure Yellows; loses gloss Retains colour and gloss

Two consequences are worth spelling out. The first is that the dose barely changes. Bisphenol A is 114.14 g/eq and HBPA is 120.19 g/eq, so a formulation that swaps one for the other on an equivalent basis moves by 5.3% – the same order of magnitude as the 1.3% step between THPA and HHPA, which is the classic case of a substitution that looks harmless on the mixing sheet. What changes is not the amount, it is the durability, the crystallinity and the colour.

The second is cost. The phenolic hydroxyl of bisphenol A is acidic enough to be run as a phenoxide and reacted directly with epichlorohydrin; a secondary alcohol is not, so hydrogenated bisphenol A epoxy resin needs a different route and carries a higher price than the aromatic version. HBPA is bought where the exterior durability is worth that premium, not as a general-purpose diol.

Not an Anhydride

HBPA turns up in hardener discussions because it is a component of the same coating and casting systems, and it is worth being blunt about the chemistry: it is a diol, not an anhydride. An anhydride cures epoxy by ring-opening against the epoxy group; an alcohol does not react with an epoxy group at a useful rate without catalysis or a temperature most shops will not run.

Role What it means in practice
Building block for hydrogenated epoxy resin Reacted in the kettle; the product sold is the glycidyl ether, not the diol
Building block for weatherable polyester Charged with diacids and other diols in a polyester cook
Chain extender for polyurethane Dosed against hydroxyl value against an isocyanate, not against an epoxy
Modifying diol in an anhydride-cured epoxy Partial replacement or add-on, used to soften the network and reduce yellowing – not as the hardener

The practical rule is simple: dose HBPA against its hydroxyl value, and dose the anhydride against its anhydride equivalent weight. Mixing the two bases is the most common arithmetic error in a formulation that contains both.

Reading the Hydroxyl Value Against the Assay

The specification gives two figures that look like two views of the same thing and are not. The hydroxyl value measures reactive equivalents; the assay measures chromatographic purity. Their ceilings differ, and the gap between them is information:

Basis Hydroxyl value Equivalent weight Reactive OH per kg
Theoretical, pure C15H28O2 466.8 mg KOH/g 120.19 g/eq 8.32 eq
Specification minimum 435 mg KOH/g 129.0 g/eq 7.75 eq
What a 96% assay implies 448.2 mg KOH/g 125.2 g/eq 7.99 eq

The hydroxyl minimum sits below what the assay minimum implies. That is not a mistake in the specification; it is a functional floor rather than a restatement of purity, and it is there to allow for the fact that not every non-HBPA molecule in the lot carries two hydroxyls. A partly hydrogenated ring carries one; a positional isomer carries two but at a different separation. The first lowers the hydroxyl value without necessarily lowering the assay by the same amount.

For any stoichiometric use – a polyester cook, a polyurethane, an acrylate ester – ask for both figures and ask which one releases the lot. A batch can pass 96% assay and still be short of reactive hydroxyl, and in a polyester that shows up as a molecular weight that will not reach target no matter how long the cook runs.

The hydroxyl value also cannot tell you the isomer ratio. HBPA is mainly the 4,4′ isomer with smaller amounts of 2,4′ and other positional and cis/trans arrangements, and every one of them is a C15H28O2 diol with the same hydroxyl value within experimental error. Isomer ratio is a chromatographic question.

Stoichiometry, Worked Once

The working equivalent weight is 129.0 g/eq at the specification floor, and 120.19 at theoretical. Using the working figure rather than the theoretical is not pedantry; it is the difference between a formulation that hits its target and one that is 7% short on hydroxyl.

Counterpart Basis HBPA per 100 parts of counterpart
Epoxy resin, EEW 185 1:1 equivalents, at 129.0 g/eq 69.7
Epoxy resin, EEW 185 1:1 equivalents, theoretical 120.19 65.0
Diacid, acid value 35 1:1 equivalents (acid equivalent 1603 g/eq) About 8
Isocyanate, NCO 23% 1:1 equivalents (5.47 eq/kg NCO) About 70.6

The epoxy line is a synthesis calculation, not a cure schedule. HBPA is reacted into the resin backbone in the kettle, or used as a partial replacement for bisphenol A in a resin cook; it is not dosed into a casting as a room-temperature hardener. The isocyanate line is the one that gets used on the plant floor, in TPU and in two-component coatings.

Moisture: Why 0.5% Is a Real Limit

Water is not inert in a polyurethane or a polyester cook. In a NCO system it consumes isocyanate and releases carbon dioxide; in a polyester cook it disturbs the glycol balance and pushes the acid value. The arithmetic for the 0.5% limit is worth doing once per project:

Item Value per 100 kg of HBPA
Water at the 0.5% limit 0.5 kg = 27.8 mol
Hydroxyl equivalents present (96% assay, OH value 435) 96 kg / 129.0 g/eq = about 744 eq
Hydroxyl equivalents consumed by that water in a NCO system 27.8 eq = 3.7%
Carbon dioxide released About 0.62 kg

So a lot sitting exactly at the moisture limit will consume almost 4% of the hydroxyl equivalents and release over half a kilogram of gas per 100 kg of charge. In a thin coating that is cosmetic; in a casting, a sealant or a foam it is a defect generator, and it is invisible on the certificate unless you look for the moisture line. Dry the diol before a polyurethane or polyester cook, and specify moisture on the purchase order rather than assuming it.

Colour: Why the Specification Says “30% in Methanol”

A high-melting solid cannot be read on the platinum-cobalt scale directly – the scale is defined for transparent liquids, and a solid has no path length to read through. The standard solution is to dissolve the product and read the solution, and the specification here says 30% in methanol. Three consequences follow, and all three matter at the point of comparison:

  • The figure is not comparable with a liquid anhydride’s neat Pt-Co value. A 30% solution reads roughly three times lighter than the equivalent body colour, so a solution limit of 30 is stricter than a neat limit of 30.
  • The solvent is part of the method. Methanol is specified because HBPA dissolves in it cleanly; reading in another solvent gives a different number for the same lot.
  • Colour drifts on storage. A diol held hot and open oxidises and the colour climbs, so a colour limit is also a statement about how the material was stored before it shipped.

Weathering: What It Fixes and What It Does Not

The hydrogenated ring removes the chromophore, which is the single largest cause of yellowing and gloss loss in an exterior clear coat or a light-coloured topcoat. It does not make a coating weatherproof on its own. A formulation still needs its ultraviolet absorber and hindered amine light stabiliser package, still needs a hydrolysis-resistant resin backbone, and still needs to be tested for the specific climate and gloss target. What HBPA changes is the starting point: a resin that does not begin yellowing from its own backbone, so the stabiliser package is fighting the environment rather than the polymer.

The same reasoning explains why HBPA appears alongside saturated, non-aromatic hardeners in the same formulations. A hydrogenated epoxy or a polyester based on HBPA is often cured with a saturated anhydride – MHHPA rather than MTHPA, for instance – for the same reason: in an exterior system, every retained double bond in the network is a potential oxidation site, and the point of paying for hydrogenation is not to reintroduce one through the hardener.

Applications

  • Weatherable saturated polyester. Powder coatings and coil coatings for exterior architectural metal; HBPA gives non-crystallinity, hydrolytic stability and colour retention in one building block.
  • Hydrogenated epoxy resins. The diol backbone of hydrogenated bisphenol A epoxy resin and its acrylate esters, for exterior coatings, can and coil coatings, and non-aromatic electrical laminates.
  • Radiation-curable monomers. Hydrogenated bisphenol A diacrylate gives low shrinkage, a modest viscosity rise and good exterior durability in UV/EB coatings and inks.
  • Polyurethane hard segments. A non-yellowing, hydrolysis-resistant chain extender for TPU, coatings and adhesives where an aromatic diol would discolour in service.
  • Modifying diol in epoxy systems. Partial replacement of bisphenol A in a resin backbone, or an add-on diol in an anhydride-cured system to soften the network and reduce yellowing.
  • Unsaturated polyester and specialty resins. A cycloaliphatic, non-crystallising diol where the aromatic chromophore is not wanted.

Storage and Handling

Supply is as a solid; the physical form – flake, pastille or ground powder – is agreed per order because it decides how the material is charged. Store sealed and dry in a cool warehouse, away from moisture, acids, isocyanates and oxidisers. HBPA is hygroscopic enough that an open bag in a humid warehouse picks up surface moisture, and the moisture specification is the first thing to be lost. Melt only in a vessel that will not overheat it; a diol held hot and open oxidises and the colour climbs.

Dust is a mechanical irritant rather than a chemical hazard at industrial hygiene levels, but use local exhaust ventilation, gloves, eye protection and a dust mask at the charging point. Spills are slippery when dry; sweep, do not wash into a drain.

Buying Checklist

  • Both hydroxyl value and assay, and which one releases the lot. The two figures are not interchangeable, and the gap between them is where a shortfall hides.
  • Moisture. 0.5% max in the specification; the figure that matters for any polyurethane or polyester use.
  • Colour basis. Pt-Co on a 30% methanol solution, and confirm the solvent method matches the one you compare against.
  • Physical form. Flake, pastille or powder – it decides the charging equipment and the dust control.
  • Isomer ratio, if the process is crystallinity-sensitive. Chromatographic rather than titrimetric, and usually declared rather than certified.
  • Regulatory statement for your market. The bisphenol A restrictions and SVHC entries are written for 80-05-7; hydrogenated bisphenol A is a different substance, but the position for a food-contact or consumer application should be confirmed with your own regulatory team rather than assumed from a specification sheet.

FAQ

Is hydrogenated bisphenol A the same as bisphenol A?

No. HBPA is 80-04-6 and bisphenol A is 80-05-7 – one digit apart, and completely different chemistry. Bisphenol A has two phenolic rings and phenolic hydroxyls; HBPA has two cyclohexane rings and secondary alcohols. They are not interchangeable in any application, and their regulatory profiles are different substances.

Is HBPA an epoxy hardener?

No, it is a diol. It is dosed against its hydroxyl value (435 mg KOH/g minimum, 129 g/eq working) and used as a building block for polyester, polyurethane and hydrogenated epoxy, or as a modifying diol in an anhydride-cured system. The hardener in such a system is the anhydride.

Why is the hydroxyl value lower than the assay suggests?

Because 435 is 93.2% of the 466.8 theoretical while the assay floor is 96%. Hydroxyl value measures reactive equivalents and assay measures chromatographic purity, and a mono-functional impurity lowers the first more than the second. Specify both for any stoichiometric application.

Why does the specification give colour on a 30% solution?

Because a high-melting solid cannot be read on the Pt-Co scale directly. The number is therefore not comparable with a liquid anhydride’s neat Pt-Co figure – a solution basis of 30 is the stricter limit.

Will HBPA make my coating weather-resistant on its own?

It removes the polymer’s own chromophore, which is the largest single cause of exterior yellowing, but a coating still needs its UV absorber and HALS package and a hydrolysis-resistant backbone. HBPA improves the starting point; it does not replace the stabiliser package.

Can HBPA replace bisphenol A one for one by weight?

No. On an equivalent basis the step is 5.3% (114.14 against 120.19 g/eq), which is small; by weight it is not a substitution at all, because the reaction chemistry differs – a phenolic hydroxyl reacts with epichlorohydrin directly, a secondary alcohol does not.

Is HBPA covered by the bisphenol A restrictions?

The restrictions and SVHC entries in force are written for bisphenol A, CAS 80-05-7. Hydrogenated bisphenol A is a different substance, but any food-contact or consumer application should be confirmed against the current rules for the destination market rather than inferred from a specification sheet.

References and Further Reading

  • CAS 80-04-6: 4,4′-(propane-2,2-diyl)dicyclohexan-1-ol; PubChem CID 94932; InChIKey CDBAMNGURPMUTG-UHFFFAOYSA-N; C15H28O2, 240.38 g/mol.
  • Hydroxyl value basis: 56110 mg KOH per mole of hydroxyl; two hydroxyls on 240.38 g gives 466.8 mg KOH/g theoretical and 120.19 g/eq. A specification value of 435 mg KOH/g corresponds to 129.0 g/eq, or 93.2% of theoretical.
  • Hydrogenation basis: bisphenol A C15H16O2 at 228.29 g/mol gains 12 hydrogen atoms to give C15H28O2 at 240.38 g/mol, a 5.3% mass increase and a 5.3% increase in equivalent weight.
  • Moisture basis: 0.5 kg of water per 100 kg is 27.8 mol; against 744 hydroxyl equivalents at the specification floor that is 3.7% of the reactive hydroxyl, releasing about 0.62 kg of carbon dioxide in a NCO system.
  • PolyBlueChem: hydrogenated bisphenol A product page; MHHPA product page; methyl nadic anhydride product page.
  • PolyBlueChem: succinic anhydride product page; anhydride dosage in phr; MTHPA vs MHHPA: tetrahydro or hexahydro.

Contact PolyBlueChem for a current certificate of analysis, a sample for resin or coating trials, and a quotation for bag, big-bag or drum supply.