Alkenylsuccinic anhydride sizing is the fastest and the most demanding of the reactive paper sizes. It gives a mill full sizing within the dryer section rather than over the following days, it works in a neutral or alkaline furnish where a rosin-alum system cannot, and in exchange it asks for an emulsification unit, a strict residence-time discipline and a chemistry team that understands what water does to an anhydride.
The constraint is not the chemistry of sizing – that part is simple and it works well. The constraint is time. Once an alkenylsuccinic anhydride is emulsified in water, the ring that does the sizing begins to open, and an open ring cannot esterify cellulose. The working life of the emulsion is measured in minutes to a few hours, and everything about how ASA is bought, stored, dosed and troubleshot follows from that single fact.
Why Neutral Papermaking Needs a Reactive Size
The classical sizing system is rosin precipitated onto the fibre with alum. It works, it is cheap, and it is locked into an acidic furnish, because the aluminium species that deposit the rosin only exist at low pH. Acidic papermaking also means acid-sensitive fillers are off the table, and the move to calcium carbonate filler – which gives higher brightness, better opacity and cheaper furnish – forced the industry to find sizes that work at pH 7 to 8.
Two chemistries answered: alkyl ketene dimer (AKD) and alkenylsuccinic anhydride (ASA). Both are reactive sizes: they do not coat the fibre, they bond to it. The bond is an ester between the size’s reactive group and a hydroxyl on the cellulose surface, and the hydrophobic tail that comes with it is what turns a hydrophilic fibre into a surface that repels water.
| Item | ASA | AKD |
|---|---|---|
| Reactive group | Anhydride ring (five-membered) | Lactone ring (four-membered, from a ketene dimer) |
| Bond formed | Ester with cellulose hydroxyl | Beta-keto ester with cellulose hydroxyl |
| Typical chain | C16 to C18 alkenyl (internal olefin derived) | C16 to C18 alkyl |
| Supply | Anhydride liquid, emulsified on site | Usually a stabilised emulsion or a solid |
| Emulsion life | Minutes to a few hours | Weeks to months |
| Sizing speed | Fast; developed in the dryers | Slow; full cure over days |
| Cure mechanism | Esterification, no further reaction needed | Requires reorganisation and time; retarded by moisture and by some fillers |
| Typical weakness | Hydrolysis, foam, deposit if the emulsion is stale | Slow cure, friction / slippage on some paper grades |
The Molecule, and Why the CAS Is a Mixture
An alkenylsuccinic anhydride is maleic anhydride with an alkenyl chain attached: a five-membered anhydride ring, one double bond, and a hydrocarbon tail that sets how hydrophobic the sized surface becomes. The sizing grades are normally built from C16 to C18 internal olefins, because internal olefins give the emulsification behaviour the machine needs while the chain is long enough to size efficiently.
The same homologous-series arithmetic that governs the epoxy grades governs these: an n-carbon chain gives a molecular weight of 14n + 98. At n = 16 that is 322; at n = 18 it is 350. Everything the mill cares about follows from that range:
| Chain length | Molecular weight | Anhydride group content | Anhydride equivalents per kg |
|---|---|---|---|
| C16 | 322 | 22.4% | 3.11 |
| C18 | 350 | 20.6% | 2.86 |
Note what that means for the certificate. A sizing grade is about 70% hydrocarbon by mass, so the “85% active content” figure on a specification is not a purity in the usual sense – it is the anhydride-bearing fraction, and the balance is carrier. Asking what the carrier is, and what the chain distribution is, matters more than asking for a higher assay.
There is no single PubChem structure for a sizing-grade CAS such as 70983-53-8, and that is not a gap in the record; it is an accurate description of the product. A mixture-grade registration covers a distribution of chain lengths, positional isomers and carriers.
The Hydrolysis Arithmetic That Sets the Whole Operation
A mole of water opens a mole of anhydride. Because the sizing-grade molecule is the heaviest in the alkenylsuccinic family, one kilogram of water destroys more of it than one kilogram of water destroys of anything else discussed on this site:
| Material | MW | Destroyed by 1 kg of water per tonne | Diacid formed |
|---|---|---|---|
| Succinic anhydride | 100.07 | 5.6 kg | 6.6 kg |
| DDSA (C12 chain) | 266.38 | 14.8 kg | 15.8 kg |
| ASA sizing grade (C16) | 322 | 17.9 kg | 18.9 kg |
| ASA sizing grade (C18) | 350 | 19.4 kg | 20.4 kg |
In a drum that arithmetic is a storage problem. In an emulsion it is the operating window, because an emulsion is mostly water: a 1% emulsion contains ninety-nine parts water to one part anhydride, and any hydrolysis at all consumes the active component. The reaction is faster warm and faster at higher pH, which is why the emulsion is made cool, used promptly, and not held overnight.
Hydrolysed ASA is not merely inactive. The diacid it becomes is surface active, so it foams in the white water system, and it can deposit on felts and in the headbox. A mill that suddenly sees foam and sizing loss together is usually looking at a stale emulsion or a leaking dilution line, not at the chemistry of the size.
Making the Emulsion
ASA is not water-soluble, so it is dispersed with a stabiliser that keeps the droplets apart and carries a cationic charge so the droplets can be retained on anionic fibre. Three stabiliser routes are in commercial use:
- Cationic starch. Cooked to a clear solution, cheap, widely available, and the traditional choice. The starch also contributes to dry strength, which is either a benefit or a nuisance depending on the grade.
- Synthetic cationic polymers. Better shear stability and a more predictable charge; higher cost, and compatibility with the rest of the wet-end chemistry has to be checked.
- Polymer-starch combinations. The usual modern compromise, tuned to the machine’s water chemistry and to the filler load.
The unit itself is a high-shear emulsifier fed with heated anhydride, stabiliser solution and dilution water, followed by a short loop to the addition point. Key operating parameters are the anhydride temperature (warm enough to flow, cool enough not to accelerate hydrolysis), the stabiliser-to-anhydride ratio, the shear, and the dilution. The residence time from emulsifier to headbox should be short enough that the emulsion reaches the fibre while most of the ring is still intact.
How the Size Is Fixed on the Fibre
The emulsion droplets are retained on the fibre by charge interaction, in competition with everything else cationic in the wet end. Once the sheet is formed, the reaction happens in the dryer section: the anhydride ring opens against a cellulose hydroxyl, an ester bond forms, and the alkenyl chain is left pointing out of the surface. Water cannot wet what the chain covers.
That is why ASA sizing is measured on the reel and not in the white water, and why the drying curve matters as much as the dose. A sheet that is under-dried has unreacted size on it; a sheet that is over-dried has size that has migrated. Both read as poor sizing, and neither is fixed by adding more emulsion.
What Actually Decides the Sizing Result
Dose is the smallest of the variables. On a real machine, the following matter more, and they are the reason two mills using the same grade get different results:
| Factor | What it does to ASA sizing |
|---|---|
| Furnish pH and alkalinity | Higher pH accelerates hydrolysis of the emulsion; the target is the neutral window, not the highest pH the filler allows |
| Filler type and loading | Precipitated or ground calcium carbonate has a large specific surface and consumes cationic species; higher filler load means more size and more retention aid |
| Anionic trash | Dissolved and colloidal anionic material consumes the cationic stabiliser before it reaches the fibre; the fix is charge control upstream, not more size |
| Retention and drainage | Size that is not retained is size wasted; first-pass retention and the retention aid programme set the efficiency |
| Conductivity and closure | A tighter white-water loop raises ionic strength, which compresses the electrostatic interaction the droplets rely on |
| Stock temperature | Warm stock shortens the already short emulsion life and changes the droplet size distribution |
| Drying | The reaction needs heat; an under-dried sheet reads as unsized |
The pattern in that table is that most ASA problems are wet-end charge problems wearing a sizing costume. A mill that adds size to fix a drainage issue, or adds retention aid to fix a sizing issue, will chase its own tail for a week.
Choosing Between ASA and AKD
The decision is usually made once per machine and revisited when grades change:
- Choose ASA where full sizing is needed quickly, where the machine has (or can justify) an emulsification unit, where grade changes are frequent and stored emulsion would be wasted, and where the friction behaviour of AKD has caused converting problems.
- Choose AKD where the machine runs long campaigns on few grades, where there is no room for an emulsification unit, where the furnish is difficult for a short-life emulsion, or where a solid or stabilised liquid size is preferred for logistics.
- Run both where the grade mix genuinely needs both behaviours – some mills use ASA for fast grades and AKD as the base load, which is an operational decision rather than a chemical one.
Troubleshooting: The Usual Suspects
| Symptom | First thing to check |
|---|---|
| Sizing drops suddenly on one grade | Emulsion age and dilution water quality; then stock temperature and pH |
| Foam in the white water with sizing loss | Hydrolysed size – stale emulsion, leaking line, or an emulsifier running hot |
| Deposits on felts or in the headbox | The same: hydrolysed ASA is surface active and deposits |
| Two-sided sizing | Uneven drying, or droplet size too large to penetrate the sheet evenly |
| Sizing fades over days | Under-cured sheet, or size that was never esterified because the ring had already opened |
| Dose creeping upward with no change | Anionic trash, closed water loop, or a filler change; check charge demand before adding more size |
Buying and Acceptance
- Active content and its basis. 85% minimum here, with the balance carrier; ask what the carrier is, because the emulsion recipe depends on it.
- Hydrolysis products. Ask how they are reported and what the limit is; pre-hydrolysed material is inactive and foams.
- Chain-length distribution. C16 to C18 is normal; the split affects emulsification and hydrophobicity, and a change of split is a reformulation even if the assay is unchanged.
- Colour. A light brown to brown liquid is normal; it ends up on white paper, so a change in shade is worth a question.
- Viscosity and feed temperature. Confirm what the emulsification unit can handle before agreeing a specification.
- Seal integrity in transit. A broken seal on a sizing drum is a rejected lot, because the failure will show up on the machine rather than in the drum.
FAQ
What does ASA stand for in papermaking?
Alkenylsuccinic anhydride. It is one of the two reactive sizes used in neutral and alkaline papermaking, the other being AKD (alkyl ketene dimer).
Why must the emulsion be used immediately?
Because the anhydride ring hydrolyses in water and a hydrolysed ring cannot esterify cellulose. The emulsion’s working life is minutes to hours depending on temperature and pH, and stale emulsion causes both sizing loss and foam.
How much water does the size tolerate?
Very little in the drum. One kilogram of water per tonne of a C16 sizing grade destroys about 17.9 kg of the anhydride. In the emulsion the arithmetic is worse because the emulsion is mostly water, which is why it is made on site and used promptly.
Can ASA be supplied as a ready-made emulsion?
Not usefully – an ASA emulsion does not survive storage. That is the structural difference from AKD, which is routinely supplied as a stabilised emulsion or a solid.
Is a sizing grade the same as the DDSA sold as an epoxy hardener?
Same chemistry, different specification. A sizing grade is defined by emulsion behaviour, hydrolysis limits and paper performance, with a chain distribution chosen for the machine. A generic epoxy-grade alkenylsuccinic anhydride is not qualified as a sizing agent.
Does ASA sizing work at acid pH?
It is designed for the neutral range. Low pH accelerates hydrolysis of the anhydride without helping the esterification, and acid furnish is the territory of rosin-alum.
What is the 85% figure on the specification?
The declared active anhydride content; the balance is carrier, and the carrier is supplier-specific. It is not a purity figure in the chromatographic sense.
References and Further Reading
- CAS 70983-53-8: alkenylsuccinic anhydride, mixture-grade registration for paper sizing; no single PubChem structure record.
- Homologous series basis: an n-carbon chain in an alkenylsuccinic anhydride gives C(n+4)H(2n+2)O3 and a molecular weight of 14n + 98, so C16 is 322 and C18 is 350.
- Anhydride content basis: C2O3 = 72.02 g/mol; 72.02 / 322 = 22.4% for C16 and 72.02 / 350 = 20.6% for C18.
- Hydrolysis basis: one mole of water per mole of anhydride; 1 kg of water per tonne is 55.5 mol, which consumes 17.9 kg of a C16 grade and forms 18.9 kg of the diacid.
- PolyBlueChem: ASA 2024 paper sizing product page; DDSA: flexibility, dose and the alkyl trap; alkenylsuccinic anhydrides: chain length and identity.
- PolyBlueChem: polyamine in papermaking: anionic trash capture; retention, drainage and pitch control; aluminium sulfate in papermaking.
Contact PolyBlueChem for a current certificate of analysis, a sample for an emulsification and machine trial, and a quotation for drum, IBC or tanker supply.