THPA (1,2,3,6-Tetrahydrophthalic Anhydride): Grades and Curing

What THPA Is, and Why One Double Bond Decides Its Use

1,2,3,6-Tetrahydrophthalic anhydride (CAS 85-43-8) is a cycloaliphatic dicarboxylic anhydride with the formula C8H8O3 and a molecular weight of 152.15 g/mol. It is made by the Diels-Alder addition of butadiene to maleic anhydride, which is why the molecule arrives with exactly one ring double bond and one anhydride group rather than with the fully saturated skeleton of its hydrogenated analogue.

That single double bond is the commercial dividing line in this family. If it stays, the molecule can be copolymerised, epoxidised or crosslinked later, and cured epoxy parts gain heat resistance. If it is hydrogenated away, the molecule becomes hexahydrophthalic anhydride, the product of choice where colour stability and weathering matter. THPA sits on the unsaturated side, and it is the workhorse anhydride for thick-section electrical casting because it gives a low exotherm, low shrinkage and a high glass transition at a reasonable cost.

Chemical and Physical Properties

Property Value
CAS Registry Number 85-43-8
IUPAC name 3a,4,7,7a-tetrahydro-2-benzofuran-1,3-dione
Common synonyms THPA; tetrahydrophthalic anhydride; 4-cyclohexene-1,2-dicarboxylic anhydride
Molecular formula C8H8O3
Molecular weight 152.15 g/mol
Anhydride groups 1 per molecule; anhydride equivalent weight 152.15 g/eq
Ring double bond 1, isolated from the anhydride ring
PubChem CID 6810
InChIKey KMOUUZVZFBCRAM-UHFFFAOYSA-N
SMILES C1C=CCC2C1C(=O)OC2=O
Appearance White flake or fused solid
Melting point About 100 deg C
Theoretical iodine value About 166.8 g I2/100 g (one double bond)
Solubility Hydrolyses in water to the diacid; soluble in many organic solvents

Two of these numbers are worth carrying in your head. The anhydride equivalent weight of 152.15 sets every dose calculation in the second half of this article. The theoretical iodine value of about 166.8 is the fingerprint of the one double bond, and it becomes a purchasing tool: a THPA lot that reads well below 166 is partly hydrogenated or blended with HHPA, while a lot that reads well above it contains something more unsaturated than THPA.

How It Is Made

The commercial route is a cycloaddition, and understanding it explains both the impurity profile and the isomer question that follows every THPA purchase order.

The Diels-Alder reaction

Butadiene (the diene) and maleic anhydride (the dienophile) combine in a concerted pericyclic reaction to give the six-membered ring with the anhydride fused to it:

C4H6 + C4H2O3 -> C8H8O3

The reaction is exothermic and needs no catalyst; it is run in a solvent or in the melt, at moderate temperature, with the diene kept in slight excess and the reactor cooled to control the exotherm. Because the product is a solid with a melting point near 100 deg C, the downstream steps are the interesting part: the reactor effluent has to be stripped of unreacted butadiene and maleic anhydride, the product has to be freed of the diacid formed by accidental hydrolysis, and the melt has to be flaked or pastillated without being held hot long enough to darken.

Why the isomer question exists

The Diels-Alder adduct is the 1,2,3,6-isomer, with the double bond isolated in the ring. Under thermal stress, or on a different reaction path, an isomer with the double bond against the anhydride ring forms: 3,4,5,6-tetrahydrophthalic anhydride, CAS 2426-02-0, with the same formula and the same molecular weight but a melting point near 67 deg C instead of 100 deg C.

Property 1,2,3,6-THPA (this product) 3,4,5,6-THPA
CAS 85-43-8 2426-02-0
InChIKey KMOUUZVZFBCRAM-UHFFFAOYSA-N HMMBJOWWRLZEMI-UHFFFAOYSA-N
Formula / MW C8H8O3 / 152.15 C8H8O3 / 152.15
Double bond position Isolated in the ring Conjugated with the anhydride ring
Melting point About 100 deg C 66 to 69 deg C

The practical consequence is that melting point is the fastest incoming check for isomer contamination, and it is the one test a buyer can run before the laboratory reports arrive. A THPA lot melting at 95 deg C or below contains a meaningful fraction of the low-melting isomer, and its free acid is usually elevated as well, because the conjugated isomer hydrolyses more readily.

Reading the Specification

Commercial THPA is sold in standard and custom grades. The standard grades are separated by assay and colour; the custom grades add free acid, ash, iron and a customer-specific anti-shrinkage compliance.

Item Why it is on the certificate
Assay 99.0% or 99.5% The residue is mostly the diacid plus oligomers; in a thick casting it changes colour and cure schedule
Colour, 80 / 60 / 30-50 Hazen Directly tied to iron content, thermal history and the colour of the cured part
Melting point 100 +/- 2 deg C Isomer identity and moisture history in a single physical measurement
Free acid 0.2% or 0.5% How much of the anhydride has already hydrolysed, i.e. how much will not react with epoxy
Ash 0.005% Inorganic residue from catalyst, rust and packaging; matters for dielectric performance
Iron 10 ppm Colour and ionic contamination; iron is the usual cause of a yellow casting
Silicon-free anti-shrinkage compliance A customer-agreed statement for processes sensitive to silicone and to cure shrinkage

The hydrolysis arithmetic behind the free-acid limit

Every anhydride group that meets water becomes a diacid, and the reaction consumes both the anhydride and the water:

C8H8O3 + H2O -> C8H10O4

The masses make the specification legible. One mole of water (18.02 g) hydrolyses one mole of THPA (152.15 g) to one mole of the diacid (170.16 g). So one kilogram of water absorbed per tonne of flake destroys about 8.4 kg of anhydride and creates about 9.4 kg of diacid, which is a free-acid figure near 0.94%.

Water absorbed per tonne Anhydride hydrolysed Free acid, as diacid Loss of anhydride equivalents
0.1 kg (0.01%) 0.84 kg About 0.09% 0.08%
1 kg (0.1%) 8.4 kg About 0.94% 0.84%
2 kg (0.2%) 16.9 kg About 1.9% 1.7%

Read the first row and the third row together. A 0.2% free-acid limit is not a formality; it corresponds to about 0.2 kg of water per tonne, which is what a sealed bag with a polyethylene liner can hold out and what a torn bag in a humid warehouse cannot. This is why the packing specification travels with the chemistry specification in any serious purchase order.

Iron, colour and the cured part

Iron at 10 ppm is the level at which a flake still reads below 30 Hazen and a casting still comes out water-white. Above that, the cured part starts to carry a yellow tint that no amount of post-cure removes, and the ion also contributes to the ionic conductivity of an insulation system. Ash below 0.005% is the same idea in a different currency: it is 50 parts per million of inorganic residue, measured because the applications that care about it are measured in parts per million rather than percent.

Anhydride Curing Chemistry

Anhydrides cure epoxy resins through a ring-opening esterification that needs heat and, usually, an accelerator. The mechanism matters because it explains the dose, the exotherm and the shrinkage behaviour that make THPA the standard choice for thick castings.

The dose

phr = (AEW / EEW) x 100 x r

AEW is the anhydride equivalent weight (152.15 for THPA), EEW is the epoxy equivalent weight of the resin, and r is the anhydride-to-epoxy molar ratio. The ratio is normally 0.85 to 1.0 because the hydroxyls generated during the reaction consume part of the anhydride, so a stoichiometric 1.0 leaves excess anhydride in the network.

Resin EEW r = 0.85 r = 0.90 r = 1.00 Note
185 (standard DGEBA) 69.9 phr 74.0 phr 82.2 phr The most common starting point
200 64.7 phr 68.5 phr 76.1 phr Lightly modified resin
250 51.7 phr 54.8 phr 60.9 phr Higher molecular weight, lower dose

Note what the table is not: it is not a weight percentage of the mix. A formulator who treats 70 phr as "70 percent" and doses on total batch weight will be wrong by roughly 40% and will produce a soft, under-cured part. The dose is always per hundred parts of resin.

The accelerator and the cure profile

Unaccelerated anhydride cure is slow. Tertiary amines such as benzyldimethylamine, substituted imidazoles and quaternary ammonium salts are the usual accelerators, added at fractions of a percent to a few percent. The gel time falls sharply with accelerator level, and so does the exotherm, which is why the accelerator is also a processing tool: it buys cycle time without buying the runaway risk of an amine-cured system.

A typical casting profile runs 2 to 4 hours at 120 to 160 deg C followed by a post-cure, and the post-cure is where the glass transition is actually developed. Skipping it gives a part that looks cured and fails a heat deflection test.

Why thick sections choose anhydride

  • Low exotherm. The reaction is far less exothermic than an amine cure, so a 100 mm casting does not self-heat into a runaway.
  • Low shrinkage. Ring-opening polymerisation builds an open network, and the volumetric shrinkage is small compared with a tight amine crosslink. This is the origin of the anti-shrinkage requirements some customers write into the specification.
  • High glass transition and good dielectrics. The ester-linked network has a high Tg and low ionic conductivity, which is why dry-type transformers and instrument transformers are almost all anhydride-cured.
  • Long pot life at melt temperature. A one-pack system of resin plus solid anhydride can be held molten for hours, which suits vacuum casting and automatic metering.

The Double Bond as a Feature

Because the double bond survives the anhydride cure, THPA opens routes that HHPA cannot:

  • Copolymerisation with styrene or acrylate monomers in unsaturated polyester and vinyl ester systems, where THPA contributes rigidity and heat resistance to the cured resin.
  • Epoxidation or hydroformylation of the ring double bond to build further functionality onto the same cycloaliphatic skeleton.
  • Further Diels-Alder chemistry, using the retained double bond as a dienophile for grafting or for thermally reversible crosslinks.
  • Post-cure crosslinking with peroxide initiators where a higher crosslink density is wanted after the epoxy network has formed.

The trade-off is stability. The unsaturated ring is also the site that oxidises and yellows, so a THPA-cured part is not the right choice for a white outdoor coating or a transparent LED encapsulant. That is a specification decision, not a quality difference.

Applications

  • Electrical casting. Dry-type transformers, instrument transformers, bushings, surge arresters, GIS insulators and sensor potting.
  • Laminates and composites. Anhydride-cured epoxy prepregs and wet-lay laminates where a long pot life and a high Tg are wanted.
  • Unsaturated polyester and alkyd resins. THPA supplies cycloaliphatic rigidity and a copolymerisable double bond.
  • Plasticiser and lubricant intermediates. Diesters made by ring opening with C4 to C10 alcohols.
  • Fine-chemical intermediate. A building block for cycloaliphatic diacids, diols and cyclic imides.

Storage, Handling and Safety

THPA is a moisture-sensitive solid that becomes corrosive on hydrolysis, and it is a skin sensitiser. Three rules cover most of the risk.

Keep it dry. Sealed bags, polyethylene liner, dry store, no open bags left over a weekend in a humid warehouse. The free-acid limit is a moisture budget, as the arithmetic above shows.

Keep it cool when molten. Melt at the lowest workable temperature, hold for the shortest workable time, and never leave a melt tank hot overnight. Hot holding darkens the product and raises the free acid.

Keep it away from amines. Anhydrides and amines react exothermically on contact. Store and dispense them in separate areas, and never share a scoop, a tray or a spill bund.

For handling, use local exhaust ventilation, gloves, eye protection and a dust mask. Clean spills dry, and never wash an anhydride spill into a drain with water: that converts a nuisance dust into a corrosive acid solution.

Buying Checklist

  1. Which grade do you actually need? 99.0% with 80 Hazen is fine for resin intermediates; 99.5% with 30 to 50 Hazen and 0.2% free acid is the electrical casting grade.
  2. Ask for the melting range, not just the melting point. A wide or low range is the first sign of isomer or moisture trouble.
  3. Ask for free acid, ash and iron together. Any one of them alone can look fine while the trio shows a wet, dirty or hot-held lot.
  4. Confirm the packing. A specification that does not name the liner is a specification that assumes the material will pick up water in transit.
  5. Confirm the InChIKey if the material is going into a regulated or critical application, because the isomer shares the formula and the molecular weight.

FAQ

Is THPA a liquid or a solid at room temperature?

A solid, melting at about 100 deg C. It is supplied as flake or as a fused solid, and it is dosed either as flake or melted in a heated vessel. The liquid anhydride in this family is MTHPA, the methyl-substituted analogue.

Can THPA be cured at room temperature?

Not as a production process. Anhydride-epoxy cure needs heat, typically 120 deg C and above with an accelerator, and a post-cure to develop the final properties.

What is the difference between THPA and MTHPA?

MTHPA is methyltetrahydrophthalic anhydride: THPA with a methyl group on the ring, which lowers the melting point into the liquid range and changes the viscosity and reactivity. MTHPA is the standard liquid anhydride for room-temperature-stable one-pack systems; THPA is the solid used where a flake or a molten solid is acceptable. Its molecular weight is 166.17 and its equivalent weight about 175.7 once the 41.0% anhydride group minimum is allowed for, which is why the dose moves by around 15% rather than by the 1.3% that separates THPA from HHPA; see MTHPA: properties, grades and cure.

Why does the specification not include a viscosity?

Because the product is a solid at ambient temperature. Viscosity becomes relevant only after melting into a resin, and at that point it is the mix viscosity that matters rather than the anhydride alone.

How much does the anhydride dose change if I switch resin?

The dose changes in proportion to the resin’s epoxy equivalent weight. Doubling the EEW halves the phr at constant r, which is why a formulation transferred to a new resin batch has to be re-dosed rather than copied.

References and Further Reading

Disclaimer: this article describes commercial specifications and industrial chemistry. Cure schedules, formulations and regulatory classifications must be validated by the user for the specific application, resin and jurisdiction.

Contact PolyblueChem for a current certificate of analysis, a sample and a quotation for THPA in flake, jumbo bag or molten form.

Scroll to Top