HHPA (Hexahydrophthalic Anhydride): Iodine Value and Cure

A Saturated Anhydride, and Why That Is the Whole Point

Hexahydrophthalic anhydride (CAS 85-42-7) is the fully hydrogenated member of the tetrahydrophthalic anhydride family: C8H10O3, 154.16 g/mol, one anhydride group and no ring double bond at all. It is a white, low-melting solid with a crystallisation point around 34 to 38 deg C, and it is bought for one dominant reason: an anhydride with no unsaturation cannot yellow.

That single fact explains its position in the market. Where a cured epoxy part has to stay water-white or has to survive ultraviolet exposure, the unsaturated anhydrides are the wrong choice regardless of how pure they are, because the ring double bond is the site that oxidises. HHPA removes that site. The cost is a slightly higher equivalent weight, a lower melting point that complicates logistics, and a hydrogenation step in the plant that the unsaturated products do not need.

Chemical and Physical Properties

Property Value
CAS Registry Number 85-42-7
IUPAC name 3a,4,5,6,7,7a-hexahydro-2-benzofuran-1,3-dione
Common synonyms HHPA; hexahydrophthalic anhydride; cyclohexane-1,2-dicarboxylic anhydride
Molecular formula C8H10O3
Molecular weight 154.16 g/mol
Anhydride equivalent weight 154.16 g/eq
Ring double bond None
PubChem CID 85689
InChIKey MUTGBJKUEZFXGO-UHFFFAOYSA-N
SMILES C1CCC2C(C1)C(=O)OC2=O
Appearance White solid, flake or fused
Crystallisation point 34 to 38 deg C
Iodine value Not more than 1.0 g I2/100 g
Colour Typically 20 Hazen or below

The Iodine Value Is the Specification

Most anhydride certificates carry an assay, a colour and a free acid. HHPA carries a fourth line, the iodine value, and it is the most informative number on the page. The reason is arithmetic.

Iodine value expresses how much iodine a material can take up, and iodine adds across carbon-carbon double bonds. A molecule of HHPA has none, so a fully hydrogenated product has an iodine value of zero. If one double bond were still present, the theoretical uptake for this molecule would be:

253.81 g I2 per mole / 154.16 g per mole x 100 = about 164.6 g I2/100 g

Measured iodine value Residual unsaturation Equivalent THPA left in the lot What it means
0.0 to 0.2 Below 0.12 mol% Below 0.12% Hydrogenation essentially complete
1.0 (specification limit) About 0.61 mol% About 0.6% At the limit; acceptable for most work
2.0 About 1.2 mol% About 1.2% Noticeable in a colour-critical casting
5.0 or above About 3 mol% About 3% Incomplete hydrogenation or a deliberate blend

Read the third column carefully, because it converts a laboratory number into a purchasing statement. Because tetrahydrophthalic anhydride has one double bond and an almost identical molecular weight, one percent of THPA in an HHPA lot raises the iodine value by about 1.67 units. So the 1.0 limit is, in effect, a limit of about 0.6% of the unsaturated isomer in the product. A supplier who reports a 99% assay and a 5.0 iodine value is telling you that roughly 3% of the lot is the yellowing-prone species, and the assay will never show it.

How the iodine value is measured

The standard methods are the Wijs and Hanus procedures, both of which add iodine monochloride or iodine bromide across the double bond and titrate the excess with thiosulphate. They are mature, cheap and reproducible, and they are the right tool for this product because the target value is near zero: the absolute value matters less than whether it is under the limit. A purchaser who wants a tighter check on a critical lot should ask for the iodine value in g I2/100 g and for the method, because the two standard methods can differ slightly at the margin.

The Crystallisation Point, and What It Says About Logistics

HHPA is described by a crystallisation point rather than a melting point, and the choice of words is deliberate. Commercial HHPA is a mixture of cis and trans isomers of the cyclohexane-1,2-dicarboxylic anhydride skeleton, so it does not have the sharp melting behaviour of a pure compound. The crystallisation point between 34 and 38 deg C reflects the isomer ratio, and two lots with identical assays can sit at different points inside that band.

Crystallisation point Reading Practical consequence
36 to 38 deg C Higher-melting isomer fraction dominant More solid handling, more heat needed to melt fully
34 to 35 deg C Lower-melting isomer fraction dominant Faster melting, but more risk of slush in transit
Below 34 deg C Out of specification; possible moisture or process deviation Reject or investigate before use

The logistics point is unavoidable: a container standing in a summer yard can exceed 40 deg C, which is above the top of this range. An HHPA shipment can therefore arrive fused, or as a drum of liquid with a solid core. The chemistry is unaffected, but the physical form is not what the customer ordered, and drawing from a partially melted drum delivers a composition that does not match the certificate. The rule on receipt is simple: if the drum is not uniformly solid or uniformly liquid, melt and homogenise before sampling.

How HHPA Is Made

HHPA is made by hydrogenating tetrahydrophthalic anhydride. The reaction is conceptually simple and operationally demanding:

C8H8O3 + H2 -> C8H10O3

The hydrogenation is run in the melt or in solution over a nickel or precious-metal catalyst at moderate pressure and temperature. The two things that decide product quality are how completely the double bond is removed, which is what the iodine value measures, and how cleanly the product is finished, which is what the colour and the assay measure. Hydrogenation that stops short leaves the unsaturated isomer in the product; hydrogenation run hot or long enough to finish the job can darken the material and increase the acid content instead.

That trade-off is why the commercial grades are separated by colour and iodine value rather than by any single purity number. A 99% assay with 20 Hazen and an iodine value of 0.3 is a different achievement from a 99% assay with 50 Hazen and an iodine value of 0.9, even though both would pass a purity specification written carelessly.

Grades and What the Custom Grade Adds

Item Grade 1 (standard) Grade 2 (custom)
Appearance White solid White solid
Assay >=99.0% >=99.5%
Colour, Hazen <=20 As agreed
Iodine value <=1.0 g I2/100 g As agreed
Crystallisation point 34 to 38 deg C As agreed
Free acid – <=0.1% or <=0.2%
Ash – <=0.005%
Silicon-free anti-shrinkage test – Compliant

The custom grade adds three things that matter in an electrical or optical casting: a free-acid ceiling of 0.1 to 0.2%, an ash limit of 0.005% and a declared silicon-free anti-shrinkage compliance. Free acid is hydrolysed anhydride and therefore lost equivalents; ash is inorganic residue that shows up in dielectric loss; the anti-shrinkage statement is a customer-agreed test for processes where cure shrinkage is measured on the finished part.

Cure Chemistry and Dose

HHPA cures epoxy exactly as the other anhydrides do, through ring opening and esterification, with heat and an accelerator. The equivalent weight is 154.16, so the dose is marginally higher than for the tetrahydrophthalic grades at the same resin:

phr = (AEW / EEW) x 100 x r, with AEW = 154.16 and r = 0.85 to 1.0

Resin EEW r = 0.85 r = 0.90 r = 1.00
185 (standard DGEBA) 70.8 phr 75.0 phr 83.3 phr
200 65.5 phr 69.4 phr 77.1 phr
250 52.4 phr 55.5 phr 61.7 phr

Compare that with the 69.9 phr that the same resin needs with THPA, and the practical message appears: switching from an unsaturated to a saturated anhydride in an existing formulation changes the dose by about 1.3% and changes the cured-part colour out of all proportion to that small number. The processing parameters carry over almost unchanged, which is why the two products are often qualified against each other in the same plant.

Accelerators are the same family used across this chemistry: benzyldimethylamine, substituted imidazoles and quaternary ammonium salts, with cure at 120 to 160 deg C and a post-cure to develop the glass transition.

Applications

  • LED and optoelectronic potting. The absence of a double bond means no yellowing path under the blue and ultraviolet flux that a LED package sees, and the low colour of the anhydride itself keeps the cured gel water-white.
  • Transparent and light-coloured castings. Instrument windows, light-guide parts, decorative castings and any part where a tint is a reject.
  • Electrical insulation. Cast transformers, sensor potting and insulators where a low exotherm, a high glass transition and low ionic content are wanted together.
  • Outdoor and weathering-resistant coatings. Powder coatings and industrial coatings cured with solid anhydride where a cycloaliphatic, saturated network resists chalking and colour drift.
  • Base material for MHHPA. Methylhexahydrophthalic anhydride is HHPA with a methyl group on the ring, and it is the liquid anhydride of choice where a one-pack system has to stay fluid at ambient temperature.
  • Polyester, alkyd and plasticiser intermediates through ring opening with alcohols.

Storage, Handling and Safety

HHPA has the same chemical hazards as the rest of the family, with one addition that deserves emphasis: it is a recognised skin and respiratory sensitiser, and the dust from flaking or bagging is the exposure route that matters. Local exhaust ventilation at the filling point, a dust mask, gloves and eye protection are baseline controls rather than optional ones.

Chemically, keep it dry. The anhydride ring hydrolyses to the diacid, and in the molten state the reaction is faster and more intimate than on a solid surface, so a covered, dry melt tank is not a refinement. Keep it away from amines, alkalis, alcohols and accelerators. Clean spills dry and dispose of them as anhydride.

Physically, keep it below its softening range. Because the crystallisation point is around 34 to 38 deg C, ordinary summer conditions can exceed it. For hot-climate destinations, specify insulated or temperature-controlled packing, and plan to re-melt and homogenise on arrival.

Buying Checklist

  1. Ask for the iodine value with the assay. A 99% HHPA with a 5.0 iodine value is not the product you want for a colour-critical part.
  2. Ask for the crystallisation point. It tells you about isomer composition and about what the shipment looked like when it arrived.
  3. Match the grade to the application. Standard 99% for general casting, the 99.5% custom grade for dielectric and optical work.
  4. Specify the packing for the climate. A 34 to 38 deg C crystallisation point plus a summer container is a fused block waiting to happen.
  5. Check the InChIKey if the material is going into a regulated application, because the family shares formulas and equivalent weights closely enough to hide a substitution.

FAQ

Is HHPA the same as MHHPA?

No. HHPA is hexahydrophthalic anhydride, a solid with a crystallisation point around 34 to 38 deg C. MHHPA is methylhexahydrophthalic anhydride, the methyl-substituted analogue, which is a liquid at ambient temperature and is used where a one-pack system has to stay fluid. They are related but not interchangeable.

Why does HHPA cost more than THPA?

Because it carries an extra hydrogenation step, and because the finishing has to deliver a low colour on top of a low iodine value. The premium buys the absence of a double bond, which is a performance property rather than a purity property.

Can I use HHPA in a hot climate?

Yes, with the right packing and the expectation that the material may arrive fused. The chemistry does not suffer; the handling does. Choose insulated or temperature-controlled containers, and re-melt and homogenise before sampling.

Does HHPA cure faster or slower than THPA?

At the same accelerator level and the same r, the difference is small. The practical differences between the two are colour stability, weathering and the possibility of later crosslinking, not gel time.

What iodine value should I write into a specification?

1.0 g I2/100 g or below for general work, and 0.5 or below where the part is colour-critical or where the material may be blended with an unsaturated anhydride later. The number is cheap to measure and it is the only line that reports residual unsaturation directly.

Is the 99.5% grade necessary for all electrical castings?

No. Most castings run on the standard grade. The custom grade exists for applications with tight dielectric loss or shrinkage requirements, and for customers whose qualification protocol was written around those limits.

Related Reading

Disclaimer: this article describes commercial specifications and industrial chemistry. Cure schedules, formulations and regulatory classifications must be validated by the user for the specific application and jurisdiction.

Contact PolyblueChem for a current certificate of analysis, a sample of either grade, and a quotation for bagged, drummed or bulk HHPA.

Scroll to Top