Acid Anhydrides: Free Acid, Colour, Iron and Moisture

Three Numbers That Describe the Same Problem

Every acid anhydride certificate carries some combination of free acid, colour and iron, and the three are usually treated as three separate line items. In practice they are one story told three ways: the material got wet, got hot, or got contaminated with metal, and each of those shows up in a different column.

This article explains what each number physically measures, how they convert into one another, what the values are worth in a plant, and what to do at the warehouse to keep them where the certificate put them.

Free Acid: Hydrolysed Anhydride

What it is. An anhydride ring opened by water becomes a dicarboxylic acid. That diacid is the "free acid" on the certificate, and it is expressed as a percentage of the corresponding diacid unless the method states otherwise:

C8H8O3 + H2O -> C8H10O4 (tetrahydrophthalic anhydride to tetrahydrophthalic acid)

Why it matters. Free acid is anhydride that will never react with epoxy. A lot at 0.5% free acid has lost 0.5% of its reactive groups before it reaches the customer, and the diacid that replaces them is a plasticising, hygroscopic species in the cured network.

The water arithmetic

The masses convert water pick-up into a free-acid figure directly. One mole of water (18.02 g) hydrolyses one mole of tetrahydrophthalic anhydride (152.15 g) to one mole of the diacid (170.16 g):

Water absorbed per tonne Anhydride destroyed Diacid formed Free acid, as diacid Anhydride equivalents lost
0.1 kg 0.84 kg 0.94 kg 0.09% 0.08%
0.5 kg 4.2 kg 4.7 kg 0.47% 0.42%
1.0 kg 8.4 kg 9.4 kg 0.94% 0.84%
2.0 kg 16.9 kg 18.9 kg 1.9% 1.7%

Two conclusions follow. First, a 0.2% free-acid specification is a moisture budget of about 0.2 kg of water per tonne, which is achievable in a sealed bag with a polyethylene liner and not achievable in a torn bag in a humid warehouse. Second, the arithmetic runs in both directions: if a delivery reads 0.9% free acid, it has taken up roughly a kilogram of water per tonne somewhere between the flaker and the customer, and the question of where is a legitimate one.

Free acid and acid value

Some certificates and most laboratories report acid value in mg KOH per gram rather than free acid in percent. For this family the conversion is a single factor, because the diacid is diprotic:

free acid % = acid value (mg KOH/g) x 0.1516 for the tetrahydrophthalic system (diacid MW 170.16)

free acid % = acid value (mg KOH/g) x 0.1534 for the hexahydrophthalic system (diacid MW 172.18)

Acid value, mg KOH/g Free acid, tetrahydro system Free acid, hexahydro system
0.66 0.10% 0.10%
1.32 0.20% 0.20%
3.30 0.50% 0.51%
6.60 1.00% 1.01%

When a certificate says "free acid 0.2% maximum" and the incoming laboratory reports an acid value of 1.5 mg KOH/g, the two are not in conflict: 1.5 x 0.1516 is 0.23%, which is a marginal fail rather than a mystery. Having the factor in the specification prevents an argument.

How the test is run

The standard method is a direct titration: dissolve the sample in a neutral solvent, titrate with alcoholic potassium hydroxide to a phenolphthalein or potentiometric end point, and calculate against the diacid equivalent. Two practical points matter for reproducibility. The solvent has to be anhydrous, because wet solvent hydrolyses more anhydride during the titration and inflates the result. And the sample should be dissolved quickly without heating, because heat plus solvent plus trace water is exactly the reaction the test is trying to measure.

Colour: What the Number Describes

Colour on an anhydride certificate is usually expressed in Hazen (APHA/Pt-Co) units for the molten or dissolved product, and occasionally in Gardner units for darker material. Both scales are visual comparisons against standard solutions, and both depend on the measurement conditions, which is why the specification should name the method as well as the limit.

Colour, Hazen What it looks like Typical cause
0 to 20 Water-white Clean process, low iron, short heat history
20 to 50 Faint straw tint Normal for the standard casting grades
50 to 80 Visible straw Longer heat history, higher iron, resin feedstock grade
Above 80 Amber Hot holding, contamination, or moisture damage

Colour is a compound indicator rather than a single measurement. It responds to iron, to thermal exposure during flaking and storage, and to moisture, because the diacid formed by hydrolysis darkens more readily than the anhydride. A lot that arrives darker than the certificate promised has usually been hot, wet or contaminated, and the free acid and iron figures should be checked before it is used in a visible part.

Iron and Ash

Iron at 10 ppm and ash at 0.005% are the two inorganic contamination limits that appear on the electrical and optical grades.

Iron is the usual cause of a yellow casting. It comes from carbon-steel melt tanks, from rust in a flaker, from unlined drums, and occasionally from the raw material. Above about 10 ppm the colour of the cured part starts to drift, and in an insulation system the ion also contributes to ionic conductivity. That is why a certificate with a 20 Hazen colour and a 30 ppm iron figure is internally consistent but unsuitable for the application it was bought for.

Ash is the inorganic residue left after combustion, so it aggregates iron, sodium, calcium, catalyst metals and any dust that entered the product. A 0.005% limit is 50 mg per kilogram, which sounds generous until it is compared with what it takes to fail a dielectric test.

Source of metal contamination Where it enters Prevention
Carbon-steel melt tanks and lines Dissolution of the oxide layer by the hot acid anhydride Stainless steel or lined equipment
Unlined or rusty drums Storage and transport Lined drums, PE inner liner
Flaker belts and scrapers Manufacturing Stainless contact surfaces, maintenance regime
Shared scoops and transfer lines Dispensing Dedicated stainless scoops and hoses
Dust and air-borne particulates Open bags in a dirty store Sealed bags, clean store, no repacking in the plant

Storage: Where the Numbers Are Actually Decided

Most of the damage described above happens after the certificate is issued. Four storage rules cover almost all of it.

1. Keep the bag sealed

A polyethylene inner liner inside a paper or woven sack is the appropriate packing, and it works only while it is intact. A bag that has been opened, partly used and folded over is a bag that is exchanging moisture with the store every day.

2. Keep the store dry and below the softening range

Humidity drives hydrolysis; temperature drives both colour and, for the low-melting products in this family, the physical form. A store that reaches 40 deg C will fuse a 34 to 38 deg C crystallisation point product and will soften a 66 to 69 deg C melting point product at the seams.

3. Run melt tanks hot for short times, and dry

Molten anhydride hydrolyses faster than solid because the water is in intimate contact rather than at the surface. A melt tank should be covered, dry, and held at the lowest workable temperature for the shortest workable time. Nitrogen blanketing is a reasonable refinement where the tank has to hold overnight.

Melt practice Effect on free acid Effect on colour
Low temperature, short hold, covered Slight rise only Minimal
High temperature, short hold Slight rise Noticeable darkening
Low temperature, long hold, open to air Steady rise through moisture pick-up Moderate darkening
High temperature, long hold, open to air Fast rise Heavy darkening

4. Segregate from amines, alkalis, alcohols and oxidisers

Anhydrides react exothermically with amines and alkalis, and react with alcohols to form esters. Sharing a spill bund, a scoop or a shelf with an amine accelerator is a contamination route that no certificate can detect afterwards.

Liquid Anhydrides: Drums, Not Bags

The four rules above are written for flake and fused solid, which is how the tetrahydro and hexahydro grades travel. The liquid members of the family – MTHPA is the volume example – fail differently, and the rules translate rather than apply unchanged.

What changes in a drum

  • Moisture exposure per opening, not per tonne. A sealed bag exchanges nothing; a drum that is opened weekly exchanges its headspace with the plant air every time. The free acid in a drum is a record of how many times it was opened as much as of how wet the store is.
  • Crystallisation, not fusion. A 0 deg C grade in an unheated store crystallises, and the crystals and the mother liquor are not the same composition. The drum must be fully melted and homogenised before sampling, or the sample describes one fraction rather than the lot.
  • Iron comes from the container. An unlined carbon-steel drum or a scratched lining moves a light-coloured liquid past its Pt-Co limit within a few weeks. A colour specification on a liquid anhydride is partly a packaging specification.
  • Heat history is not reversible. Re-melt in a controlled oven or with a drum heater at the lowest workable temperature. An open flame or a high-temperature band heater will move colour and free acid at the same time, and neither comes back.

The water arithmetic is slightly harsher for the liquid

The conversion used on this page, 0.94 points of free acid per 0.1% of water, is the figure for the smaller THPA molecule at 152.15. For MTHPA at 166.17, one kilogram of water per tonne destroys about 9.2 kg of anhydride and forms about 10.2 kg of the diacid, which reads as about 1.0 point. The difference is 8%, and it only matters at the tight end: a 0.1% free acid limit is a moisture budget of about 0.1 kg per tonne, which is a nitrogen-blanket requirement rather than a handling preference.

Where a drum is specified at 0.1 or 0.2% free acid, blank with dry nitrogen or dry air after partial use, keep the working container small, and give the drum one owner. A 0.1% drum opened by everyone in the plant is a 0.5% drum by the end of the year, and the certificate will still say 0.1%.

The grading, colour and viscosity axes of the liquid product are set out in MTHPA grades, and the hydrolysis and storage chemistry in the MTHPA main article.

The highest-viscosity member: MNA

Methyl nadic anhydride (25134-21-8, 178.18) is the largest molecule on this page’s liquid list, so it pays the most per unit of water: one kilogram of water per tonne destroys about 9.9 kg of anhydride and forms about 10.9 kg of the C10H12O4 diacid, which reads as about 1.09 points of free acid. Reverse conversion: free acid percent equals acid value multiplied by 0.1748, the largest factor in the family – which means the same acid value represents more damage than it would on a THPA certificate.

It also samples differently. At 170 to 300 mPa.s, MNA has to be warmed and homogenised before a sample is taken, because the isomer mixture that produces the viscosity band does not separate evenly. A sample pulled from the top of a cold drum can describe one fraction of the lot rather than the lot, and the Pt-Co reading that comes back will be that fraction’s colour. See MNA (CAS 25134-21-8) and the MNA main article.

The heavier the molecule, the more water costs

The conversion on this page starts from a fixed number of moles: one kilogram of water per tonne is 55.5 moles, and each mole opens one mole of anhydride. The heavier the anhydride, the more kilos one kilogram of water therefore destroys.

Anhydride Molecular weight Destroyed by 0.1% water Free acid rise
Succinic anhydride 100.07 5.6 kg/t +0.66 points
THPA 152.15 8.4 kg/t +0.94 points
MNA 178.18 9.9 kg/t +1.09 points
DDSA 266.38 14.8 kg/t +1.58 points
ASA sizing grade, C16 about 322 17.9 kg/t –

For the long-chain alkenylsuccinic anhydrides this changes the storage rule rather than just the arithmetic: a DDSA drum has half the moisture budget of a THPA drum for the same free acid limit. The extreme case is the paper-sizing grades, which are emulsified in water and used within minutes – see the ASA sizing article.

There is a second degradation route that the solid grades do not have. An alkenyl chain has allylic hydrogens next to the double bond, and those are the weakest bonds in the molecule; oxygen attacks them first, the hydroperoxides decompose into carbonyls, and the colour moves while assay and free acid stay in specification. The saturated analogue has no such position – which is why DDSA is sold with a yellow colour band and its hydrogenated twin with a colourless to pale yellow one.

Incoming Inspection in Ten Minutes

  1. Appearance and form. Flake, fused block, or liquid? A fused block in a hot climate is expected; a fused block in a cool climate is a signal.
  2. Melting or crystallisation range. The cheapest identity and moisture check available.
  3. Colour against a standard on a molten or dissolved sample, using the method named in the specification.
  4. Acid value or free acid by titration. The number that tells you whether the material got wet between the plant and your store.
  5. Iodine value for the hydrogenated products, because it is the only direct measure of residual unsaturation.
  6. Retain a sealed sample of every lot, labelled with the batch, for at least the shelf life quoted to your own customer.

FAQ

How fast does free acid rise in an open bag?

It depends on the humidity and the exposed surface area, and it is not linear: the surface hydrolyses first and then slows as the diacid layer forms. In a humid store the difference between a sealed and an open bag becomes visible on the certificate within weeks, which is why the packing specification is part of the chemistry specification.

Can free acid be reduced before use?

Not practically. The diacid cannot be converted back to the anhydride without a chemical step, and distilling the anhydride away from the diacid is a manufacturing operation rather than a plant one. The lot is what it is; that is why the incoming test matters.

Does colour matter if my part is not visible?

Less, but not never. Colour correlates with thermal history and with iron, and iron correlates with dielectric loss. A dark lot in a hidden electrical casting is usually acceptable; the same lot in a thin section may not be.

Is a nitrogen blanket necessary on a melt tank?

Not strictly, but it is cheap insurance on a tank that is held hot overnight. The blanket excludes the humid air that would otherwise sit on the melt surface and feed hydrolysis.

What is the difference between acid value and free acid?

The same thing in different units. Acid value reports the milligrams of potassium hydroxide neutralised per gram of sample; free acid reports the percentage of the corresponding diacid. The conversion factor for the tetrahydrophthalic system is about 0.1516, so an acid value of 1.32 mg KOH/g is a free acid of about 0.20%.

How should an anhydride spill be cleaned?

Dry, with an inert absorbent, and disposed of as anhydride. Never wash it into a drain: water converts the spill into a corrosive acid solution and spreads it beyond the bund.

Related Reading

Disclaimer: this article describes analytical practice and storage handling for acid anhydrides. Test methods and acceptance limits must be agreed between buyer and supplier, and handling must follow the current safety data sheet and local regulations.

Contact PolyblueChem for a certificate of analysis with free acid, colour, iron and ash reported together, and for packing options matched to your climate.